<p class="0" style="line-height: 200.0%;text-indent: -25.3pt;margin-top: 13.0px;margin-bottom: 1.0px;margin-left: 33.0px;"><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">□ </span><span style="font-size: 15.0pt;">국립소방연구원</span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">(</span><span style="font-size: 13.0pt;">원장 이창섭</span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">)</span><span style="font-size: 15.0pt;">은 단열벽지</span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">(</span><span style="font-size: 13.0pt;">폼블럭</span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">)</span><span style="font-size: 15.0pt;">를 시험 분석한 결과 가연성이 높고 화염전파속도가 빨라 화재위험성이 높으므로 사용에 주의가 필요하다고 밝혔다</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">.</span></p> <p class="0" style="line-height: 200.0%;text-indent: -31.8pt;margin-top: 13.0px;margin-bottom: 1.0px;margin-left: 42.0px;"><span style="font-size: 15.0pt;"> </span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">○ </span><span style="font-size: 15.0pt;">단열벽지</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">(</span><span style="font-size: 13.0pt;">폼블럭</span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">)</span><span style="font-size: 15.0pt;">는 벽돌로 쌓아놓은 모양의 합성수지 벽지로 단열성능이 뛰어나고 시공이 간편해 일반 가정집에 많이 부착되어 있다</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">.</span></p> <p class="0" style="line-height: 200.0%;text-indent: -31.1pt;margin-top: 13.0px;margin-bottom: 1.0px;margin-left: 41.0px;"><span style="font-size: 15.0pt;"> </span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">○ </span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">2018</span><span style="font-size: 15.0pt;">년 수원 골든프라자에서 화재가 발생해 </span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">1</span><span style="font-size: 15.0pt;">명이 사망하고 </span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">66</span><span style="font-size: 15.0pt;">명이 부상하였는데 통로에 단열벽지가 설치되어 있었다</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">. </span><span style="font-size: 15.0pt;">이처럼 대형화재 현장에 단열벽지</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">(</span><span style="font-size: 13.0pt;">폼블럭</span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">)</span><span style="font-size: 15.0pt;">가 부착돼 있는 경우가 종종 발견되므로 국립소방연구원에서 시험을 통해 화재위험성을 분석했다</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">. </span></p> <p class="0" style="line-height: 200.0%;text-indent: -24.8pt;margin-top: 13.0px;margin-bottom: 1.0px;margin-left: 33.0px;"><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">□ </span><span style="font-size: 15.0pt;">시험은 단열벽지</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">(</span><span style="font-size: 13.0pt;">폼블럭</span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">)</span><span style="font-size: 15.0pt;">의 </span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">① </span><span style="font-size: 15.0pt;">연소시 발생하는 열량</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">, </span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">② </span><span style="font-size: 15.0pt;">평균연소지속열</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">, </span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">③ </span><span style="font-size: 15.0pt;">방염성능을 시중에 판매되는 일반벽지 및 방염벽지와 비교하는 형태로 진행했다</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">.</span></p> <p class="0" style="line-height: 200.0%;text-indent: -33.1pt;margin-top: 13.0px;margin-bottom: 1.0px;margin-left: 44.0px;"><span style="font-size: 15.0pt;"> </span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">○ </span><span style="font-size: 15.0pt;">연소 시 발생되는 열량</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">*</span><span style="font-size: 15.0pt;">은 단열벽지</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">(</span><span style="font-size: 13.0pt;">폼블럭</span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">)</span><span style="font-size: 15.0pt;">가 </span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">11.2 MJ/</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">㎡</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">**</span><span style="font-size: 15.0pt;">로 방염벽지</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">(</span><span style="font-size: 15.0pt;">평균 </span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">3.3 MJ/</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">㎡</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">) </span><span style="font-size: 15.0pt;">및 일반벽지</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">(</span><span style="font-size: 15.0pt;">평균 </span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">2.0 MJ/</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">㎡</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">)</span><span style="font-size: 15.0pt;">에 비해 월등히 높아 화재 확대 위험성이 높았다</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">.</span></p> <p class="0" style="line-height: 200.0%;text-indent: -31.5pt;margin-top: 13.0px;margin-bottom: 1.0px;margin-left: 42.0px;"><span style="font-size: 13.0pt;"> </span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">*</span><span style="font-size: 13.0pt;">연소 시 발생되는 열량이 높으면 화재위험성이 커진다</span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">.</span></p> <p class="0" style="line-height: 200.0%;text-indent: -31.5pt;margin-top: 13.0px;margin-bottom: 1.0px;margin-left: 42.0px;"><span style="font-size: 13.0pt;"> </span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">**1</span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">㎡</span><span style="font-size: 13.0pt;">당 발생되는 열량의 단위</span></p> <p class="0" style="line-height: 200.0%;text-indent: -31.1pt;margin-top: 13.0px;margin-bottom: 1.0px;margin-left: 41.0px;"><span style="font-size: 15.0pt;"> </span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">○ </span><span style="font-size: 15.0pt;">평균연소지속열</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">* </span><span style="font-size: 15.0pt;">또한 단열벽지</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">(</span><span style="font-size: 13.0pt;">폼블럭</span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">)</span><span style="font-size: 15.0pt;">가 </span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">0.3 MJ/</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">㎡</span><span style="font-size: 15.0pt;">로 방염벽지</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">(3.4 MJ/</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">㎡</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">) </span><span style="font-size: 15.0pt;">및 일반벽지</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">(2.5 MJ/</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">㎡</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">)</span><span style="font-size: 15.0pt;">보다 낮아 화재발생시 화염 전파가 빠른 것으로 나타났다</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">.</span></p> <p class="0" style="line-height: 200.0%;text-indent: -21.5pt;margin-top: 13.0px;margin-bottom: 1.0px;margin-left: 28.0px;"><span style="font-size: 15.0pt;"> </span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">*</span><span style="font-size: 13.0pt;">시료의 연소가 지속되기 위하여 필요한 단위면적당 평균 열량을 말하며</span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">, </span><span style="font-size: 13.0pt;">값이 낮을수록 화염전파속도가 빠르다는 것을 의미한다</span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">.</span></p> <p class="0" style="line-height: 200.0%;text-indent: -30.2pt;margin-top: 13.0px;margin-bottom: 1.0px;margin-left: 40.0px;"><span style="font-size: 15.0pt;"> </span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">○ </span><span style="font-size: 15.0pt;">방염</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">*</span><span style="font-size: 15.0pt;">성능시험 결과 방염벽지는 방염성능이 있지만 단열벽지</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">(</span><span style="font-size: 13.0pt;">폼블럭</span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">)</span><span style="font-size: 15.0pt;">와 일반벽지는 방염성능이 없었다</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">.</span></p> <p class="0" style="line-height: 200.0%;text-indent: -30.2pt;margin-top: 13.0px;margin-bottom: 1.0px;margin-left: 40.0px;"><span style="font-size: 13.0pt;"> </span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">*</span><span style="font-size: 13.0pt;">가연성 물품의 연소를 지연시키기 위하여 화학처리를 하는 것 </span></p> <p class="0" style="line-height: 200.0%;text-indent: -22.9pt;margin-top: 13.0px;margin-bottom: 1.0px;margin-left: 30.0px;"><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">□ </span><span style="font-size: 15.0pt;">분석 결과 단열벽지</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">(</span><span style="font-size: 13.0pt;">폼블럭</span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">)</span><span style="font-size: 15.0pt;">는 발생 열량이 높고 화염 전파속도가 빨라 화재 확산의 주요 원인으로 작용할 수 있었다</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">.</span></p> <p class="0" style="line-height: 200.0%;text-indent: -27.0pt;margin-top: 13.0px;margin-bottom: 1.0px;margin-left: 36.0px;"><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">□ </span><span style="font-size: 15.0pt;">이창섭 국립소방연구원장은 단열벽지</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">(</span><span style="font-size: 13.0pt;">폼블럭</span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">)</span><span style="font-size: 15.0pt;">는 화재위험성이 높아 이를 사용함에 있어서는 주의가 필요하며</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">, </span><span style="font-size: 15.0pt;">특히 화재발생시 피난이 어려울 수 있으므로 현관문과 같은 출입 통로에 단열벽지</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">(</span><span style="font-size: 13.0pt;">폼블럭</span><span style="letter-spacing: 0.0pt;font-size: 13.0pt;">)</span><span style="font-size: 15.0pt;">를 부착하는 것은 자제해야 한다고 당부했다</span><span style="letter-spacing: 0.0pt;font-size: 15.0pt;">.</span></p> <div class="hwp_editor_board_content" id="hwpEditorBoardContent"><br /></div>

국립소방연구원(원장 이창섭)은 단열벽지(폼블럭)를 시험 분석한 결과 가연성이 높고 화염전파속도가 빨라 화재위험성이 높으므로 사용에 주의가 필요하다고 밝혔다.

단열벽지(폼블럭)는 벽돌로 쌓아놓은 모양의 합성수지 벽지로 단열성능이 뛰어나고 시공이 간편해 일반 가정집에 많이 부착되어 있다.

2018년 수원 골든프라자에서 화재가 발생해 1명이 사망하고 66명이 부상하였는데 통로에 단열벽지가 설치되어 있었다. 이처럼 대형화재 현장에 단열벽지(폼블럭)가 부착돼 있는 경우가 종종 발견되므로 국립소방연구원에서 시험을 통해 화재위험성을 분석했다.

시험은 단열벽지(폼블럭)연소시 발생하는 열량, 평균연소지속열, 방염성능을 시중에 판매되는 일반벽지 및 방염벽지와 비교하는 형태로 진행했다.

연소 시 발생되는 열량*은 단열벽지(폼블럭)11.2 MJ/**로 방염벽지(평균 3.3 MJ/) 및 일반벽지(평균 2.0 MJ/)에 비해 월등히 높아 화재 확대 위험성이 높았다.

*연소 시 발생되는 열량이 높으면 화재위험성이 커진다.

**1당 발생되는 열량의 단위

평균연소지속열* 또한 단열벽지(폼블럭)0.3 MJ/로 방염벽지(3.4 MJ/) 및 일반벽지(2.5 MJ/)보다 낮아 화재발생시 화염 전파가 빠른 것으로 나타났다.

*시료의 연소가 지속되기 위하여 필요한 단위면적당 평균 열량을 말하며, 값이 낮을수록 화염전파속도가 빠르다는 것을 의미한다.

방염*성능시험 결과 방염벽지는 방염성능이 있지만 단열벽지(폼블럭)와 일반벽지는 방염성능이 없었다.

*가연성 물품의 연소를 지연시키기 위하여 화학처리를 하는 것

분석 결과 단열벽지(폼블럭)는 발생 열량이 높고 화염 전파속도가 빨라 화재 확산의 주요 원인으로 작용할 수 있었다.

이창섭 국립소방연구원장은 단열벽지(폼블럭)는 화재위험성이 높아 이를 사용함에 있어서는 주의가 필요하며, 특히 화재발생시 피난이 어려울 수 있으므로 현관문과 같은 출입 통로에 단열벽지(폼블럭)를 부착하는 것은 자제해야 한다고 당부했다.